STRENGTH PROPERTIES AND MICROSTRUCTURAL CHARACTERIZATION OF METAKAOLIN GEOPOLYMER CONCRETE SYNTHSIZED AT AMBIENT TEMPERATURE
Loading...
Date
Journal Title
Journal ISSN
Volume Title
Publisher
ARID ZONE JOURNAL OF ENGINEERING, TECHNOLOGY & ENVIRONMENT
DOI
Abstract
Geopolymer concrete has been gaining extensive attention in recent years due to its
numerous advantages over Ordinary Portland cement concrete in terms of reduced
carbon footprint, improved mechanical strength, durability as well as chemical
resistance. However, production of geopolymer concrete is usually affected by several
factors such as the synthesis temperature, nature of the source material and the type
of alkaline activator used. For these materials to have wider application within the
Nigerian construction industry, there is a need to synthesize the concrete at ambient
temperature and to examine the suitability of native Alkaleri kaolin to produce
geopolymer concrete. The study presents the strength and microstructural properties of
Metakaolin Geopolymer Concrete synthesized at ambient temperature. Alkaleri
calcined kaolin from Bauchi state Nigeria was used as the main geopolymer precursor
with sodium hydroxide and sodium silicate as the alkaline activating agent. The
Geopolymer concrete was prepared with Silicon/Aluminium ratio of 2.0 and 2.5
(Geopolymer concrete M1 and M2 respectively) and cured for 3, 7, 14, 28, and 90
days at ambient condition (average temperature of 26°C and average relative humidity
of 61± 15%). Fourier Transform Infra-Red, X-ray Diffraction, Thermo-Gravimetric
Analysis, Scanning Electron Microscopy as well as compressive strength and split tensile
strength test were conducted on the Geopolymer concrete at appropriate curing age to
examine their microstructure and strength properties. The Fourier Transform Infra-Red
revealed that there was an immediate geopolymeric reaction between the metakaolin
and the alkali activator. The X-ray Diffraction showed that the raw metakaolin sample
and both Geopolymer concrete M1 and M2 were amorphous in nature; while the
Geopolymer concrete M2 (Silicon/Aluminium ratio of 2.5) exhibited good dissolution of
the kaolinite which resulted in a more compact and stable structure in comparison with
Geopolymer concrete M1 (Silicon/Aluminium ratio of 2.0). This was also confirmed by
the Scanning Electron Microscopic images of the Geopolymer concretes. The Thermo Gravimetric Analysis revealed that both Geopolymer concrete M1 and M2 were
thermally stable at 300°C and at 800°C, only the organic phase of the geopolymer
decomposed. The strength properties (compressive and tensile strength) of Geopolymer
concrete M1 and M2 increased with increase in the curing age, and Geopolymer
concrete M2 displayed slightly higher strength in all the curing ages as compared with
the Geopolymer concrete M1. This implies that the higher the Silicon/Aluminium ratio,
the higher the mechanical strength of the geopolymer. Both the Geopolymer concrete
samples attained a compressive strength that can be acceptable for structural use as
normal strength concrete grade C20/25 as specified in the requirement of BS EN 206-
1 2000 at 28 days curing