Gmelina arborea sawdust was chemically modified using 4% and 8% concentrations of
NaOH solution for 30 and 90 minutes soaking times. The influence of this modification on
the chemical composition and thermal properties of samples were investigated. Chemical
characterization of samples revealed that the percentage content of hemicelluloses
decreased from 24.5% in the unmodified sample to 20.8% in samples soaked in 4%
NaOH solution for 90 minutes. A further decrease to 17.6% and 15.2% was observed
when samples were treated with 8% NaOH for 30 and 90 minutes, respectively. The
amount of lignin decreased from 25.0% in unmodified samples to 19.0% when the sample
was treated with 8% NaOH for 90 minutes. A moisture content of 9.0% and 2.5% were
recorded in unmodified and sample treated with 8% NaOH for 90 minutes, respectively.
However, the cellulose content increased from 38.1% in unmodified sample to 60.1%
when the sample was treated with 8% NaOH for 90 minutes. The percentage weight loss
increased as concentration and modification time increased. Functional groups analysis
by Fourier Transform Infrared Spectroscopy (FTIR) showed evidence of reduction in OH
and removal of C=O groups associated with the wood polymers after chemical
modification. Thermogravimetric analysis revealed that samples treated with 4% NaOH
for 90 minutes presented the highest onset and peak degradation temperatures of
274.0°C and 372.1°C, respectively. From these results, it can be concluded that
modification with 4% NaOH solution for 90 minutes imparted a significant improvement